Coating Peeling in Roll Forming: 7 Root Causes From Coil to Panel

Why a Coating That Passes on Flat Sheet Peels at the Roll

Adhesion tests on flat sheet measure a bond at zero strain. Roll forming does not run at zero strain. At the outer radius of a bend, the steel elongates and the film bonded to it must elongate by the same amount. On a tight rib that strain reaches 10 to 20 percent, applied in a fraction of a second. That gap explains why a coil that passes a cross-hatch test at 5B and a T-bend at 1T can still show paint lifting at the rib corner.

Read the Failure Surface First

What sits under the flake tells you which interface failed. Bare grey steel with no zinc points to pretreatment or primer to substrate. Bright zinc with no primer residue points to primer cure. Primer on the steel with topcoat on the flake points to the intercoat. Lifted along one side points to friction at the roll face, and lifted from a cut edge points to shear burr or edge damage.

The Coil and the Coating System

Polyester topcoats cure to a peak metal temperature of 232 to 243 C, with primers lower, around 204 to 232 C. If the primer never reached its PMT, the film stays under-crosslinked and fails under forming stress even though a flat coupon passes. Over-cure embrittles the film, and a line stop with strip sitting in the oven does the same.

The Bend Radius and the Line

A 1.5 mm sheet bent to a 1.5 mm inside radius puts roughly 33 percent strain on the outer film, and no standard architectural coating survives that. Then the line can add its own damage. A roll gap set too tight turns forming into a compression test, and a rough roll face drags the film. Set gap by thickness plus 5 to 10 percent per side.

Read the full article →

Cellular Floor Deck Roll Forming: 6 Double-Line Techniques

Two Coils Set the Whole Line Cellular production starts with developed strip width, not tonnage. The deck coil must yield the rib geometry,...